The process optimization of the retention ring mold was highly involved; from the first part, it was clear a major redesign was in order. There was simply no way that the retention ring would fit within the outer diameter of the Yo-yo body and initially it was unclear as to whether this was the result of an error in design or in fabrication.
The design of the original retention ring mold had been dictated by the location of ejector pins. This aspect of the design worked very well, as there was no difficulty removing the finished part from the mold. Unfortunately, this also prevented any alteration of the diameter of the ring without designing an entirely new mold and ejection system. Despite the amount of work and machining this presented, it was decided that it would be better to make an alteration to the ring than it would to the body of the yo-yo, which would have to be expanded dramatically to accept the larger diameter ring.
We changed the mold to a thinner ring by decreasing the outer diameter, and installed a runner system to a larger diameter ejection ring that ran at a radius that transected the sprue (see figure below). The principle was that an outer ring of ejector pins would strike the removal ring, and in the process the retention ring at its center clear of the mold. Though this created visual defects in 3 places rather than one on the ring, it was of little concern as the outer walls of the ring would be hidden anyways.
From the first test, we observed a somewhat unexpected behavior. The thin outer ring intended to be struck by the ejector pins was cooling significantly more rapidly than the retention ring its self. This meant that for short cooling times, the ring had a tendency to stick to the cavity mold and would pull the retention ring most of the way clear, leaving the rest of the work to the sprue ejector pin. As cooling time increased, the retention ring began to hold more resolutely and removal became difficult. The thin runners to the outer ring would shear on impact, leaving the retention ring wedged. Accordingly we kept the cooling time at a relatively short 9 seconds, with a 4 second screw feed delay time.
Testing our finished retention ring, we found that we had underestimated the degree of shrinkage, and the ring dropped easily into the Body of the yo-yo. Luckily, this had been expected in our original design, and the interference provided by the body could be adjusted by a simple turning operation. The outer diameter of the body core mold was progressively turned down until a strong interference fit was achieved.
Pressing the ring was difficult, and required the added force of an arbor press. This was good, as it means that we will likely avoid the risk of spilling ball bearings even if the yo-yo were to be dropped or thrown.
With regards to the body, it was discovered later that an outdated drawing had been used to create the mold. This explained the original difficulty of fitting the ring. This also resulted in a string gap that was larger than expected, and a problem by which the string would slip next to the bearing and bind. Both of these problems were solved by inserting a small brass shim behind the magnet that was holding our nut guide into the mold. This decreased the string gap, and held the bearing in closer proximity to the sides of the yo-yo, preventing the string from slipping.
Ejection of the body with wider walls was initially disastrous due to the degree by which the walls clamped to the core mold. After trying a variety of cooling times ranging from 9-35 seconds, it was determined that slowing the ejector speed to 15%, and ejection force to 45% was sufficient to remove the part without either blowing out or severely deforming the back.
No changes were needed for the Spokes or the Cover.
No comments:
Post a Comment